POM 美國(guó)LNP KF002L 低氣味POM GF10增強(qiáng)
LNP THERMOCOMP KF002L is a compound based on Acetal Homopolymer resin containing 10% Glass Fiber. Added features of this material include: Low Extractible.
LNP THERMOCOMP KF002L是一種基于含10%玻璃纖維的縮醛均聚樹脂的化合物。這種材料的附加特性包括:低提取率。
葉生13925706091
KF002L物性表:
REVISION: 04/02/2020 Compare this region | ||||
---|---|---|---|---|
PROPERTIES | TYPICAL VALUES | UNITS | TEST METHODS | |
MECHANICAL | ||||
Tensile Stress, yield | 66 | MPa | ASTM D 638 | |
Tensile Stress, break | 63 | MPa | ASTM D 638 | |
Tensile Strain, yield | 2.2 | % | ASTM D 638 | |
Tensile Strain, break | 3.4 | % | ASTM D 638 | |
Tensile Modulus, 50 mm/min | 6200 | MPa | ASTM D 638 | |
Flexural Stress | 103 | MPa | ASTM D 790 | |
Flexural Modulus | 4820 | MPa | ASTM D 790 | |
Tensile Stress, yield | 65 | MPa | ISO 527 | |
Tensile Stress, break | 63 | MPa | ISO 527 | |
Tensile Strain, yield | 2.1 | % | ISO 527 | |
Tensile Strain, break | 3.2 | % | ISO 527 | |
Tensile Modulus, 1 mm/min | 5600 | MPa | ISO 527 | |
Flexural Stress | 105 | MPa | ISO 178 | |
Flexural Modulus | 4400 | MPa | ISO 178 | |
IMPACT | ||||
Izod Impact, unnotched, 23°C | 384 | J/m | ASTM D 4812 | |
Izod Impact, notched, 23°C | 42 | J/m | ASTM D 256 | |
Instrumented Impact Energy @ peak, 23°C | 6 | J | ASTM D 3763 | |
Multiaxial Impact | 2 | J | ISO 6603 | |
Izod Impact, unnotched 80*10*4 +23°C | 26 | kJ/m2 | ISO 180/1U | |
Izod Impact, notched 80*10*4 +23°C | 4 | kJ/m2 | ISO 180/1A | |
THERMAL | ||||
HDT, 0.45 MPa, 3.2 mm, unannealed | 162 | °C | ASTM D 648 | |
HDT, 1.82 MPa, 3.2mm, unannealed | 155 | °C | ASTM D 648 | |
CTE, -40°C to 40°C, flow | 1.08E-05 | 1/°C | ASTM E 831 | |
CTE, -40°C to 40°C, xflow | 5.4E-06 | 1/°C | ASTM E 831 | |
CTE, -40°C to 40°C, flow | 1.12E-04 | 1/°C | ISO 11359-2 | |
CTE, -40°C to 40°C, xflow | 6.05E-05 | 1/°C | ISO 11359-2 | |
HDT/Bf, 0.45 MPa Flatw 80*10*4 sp=64mm | 162 | °C | ISO 75/Bf | |
HDT/Af, 1.8 MPa Flatw 80*10*4 sp=64mm | 148 | °C | ISO 75/Af | |
PHYSICAL | ||||
Density | 1.49 | g/cm3 | ASTM D 792 | |
Moisture Absorption, 50% RH, 24 hrs | 0.2 | % | ASTM D 570 | |
Mold Shrinkage, flow, 24 hrs | 1.6-1.8 | % | ASTM D 955 | |
Mold Shrinkage, xflow, 24 hrs | 1.5-1.7 | % | ASTM D 955 | |
Mold Shrinkage, flow, 24 hrs | 1.7 | % | ISO 294 | |
Mold Shrinkage, xflow, 24 hrs | 1.6 | % | ISO 294 | |
Density | 1.49 | g/cm3 | ISO 1183 | |
INJECTION MOLDING | ||||
Drying Temperature | 80 | °C | ||
Drying Time | 4 | hrs | ||
Melt Temperature | 200-215 | °C | ||
Front - Zone 3 Temperature | 210-220 | °C | ||
Middle - Zone 2 Temperature | 195-205 | °C | ||
Rear - Zone 1 Temperature | 175-190 | °C | ||
Mold Temperature | 80-110 | °C | ||
Back Pressure | 0.2-0.3 | MPa | ||
Screw Speed | 30-60 | rpm |